Hobart Welding Products 3545-20 manual Gmaw MIG Aluminum Welding Hints, Before You Start Welding

Page 23

5-5. GMAW (MIG) Aluminum Welding Hints

Here are several hints to help you be more successful with your new aluminum feed system.

MIG welding aluminum requires different techniques than MIG welding mild steel.

A. Before You Start Welding

SMaterial thickness that can be welded with MIG process or aluminum are 14 ga. [0.074 in. (1.9 mm)] or heavier. (How heavy depends on the output capacity of the welder being used.) To MIG weld aluminum thinner than 14 ga. either specialized pulsed MIG or AC TIG welding equipment may be necessary.

SThe removal of lubricants from the aluminum base material may be necessary. Consult with your local welding distributor for their recommendation on aluminum cleaners.

SOxide removal should be done after degreasing. This should be done with a stainless steel wire brush. This can be done with a hand wire brush or with a cup wire brush. If a power wire brush is used, keep the RPM’s and pressures low to reduce smearing the surface of the material, which could entrap oxides and impurities under the surface. Always use a wire brush that is used only on aluminum to keep from contaminating the base material.

SContact you local welding distributor or aluminum filler metal representative for recommendations on wire alloys that fit your application. Know the alloy of your base aluminum and what conditions the finished part will be subjected to. The two most readily available aluminum filler wires are ER4043 and ER5356.

B. Welding Techniques

SMake sure the welding power source is set up to weld DCEP (DC Electrode Positive).

SFor MIG welding aluminum you need to use a 10 to 15 degree push travel angle (tip and nozzle pointing in the direction of travel). See Figure 5-1.

Side View Of Gun Tip Angle

10°-15°10°-15°

Direction Of Welding

 

Forehand (Push)

Backhand (Drag)

Technique

Technique

Figure 5-1. Gun Tip Angle

SPulling or using a drag angle will produce porous, dirty welds due to a lack of gas coverage.

SSpray transfer is the desired mode of metal transfer for welding aluminum. The spray transfer is a very smooth transfer of molten metal droplets from the end of the electrode to the molten pool. The droplets crossing the arc are smaller in diameter than the electrode. There is no short-circuiting in spray transfer. With spray transfer, the deposition rate and efficiency is relatively high. The arc is very smooth, stable, and stiff and the weld bead has a nice appearance and a good wash into the sides. In the spray transfer, a large amount of heat is involved which creates a large pool with good penetration that can be difficult to control and cannot be used on materials thinner than 14 ga. This transfer will produce a hissing sound and no spatter.

SThe short arc transfer on aluminum produces poor cleaning action, poor tie-in at the edges of the weld, and large amounts of spatter and smoke.

SThe reflective heat and weld puddle that is present when MIG welding aluminum is very hot. Holding the tip closer than 3/4 in. could lead to the wire burning back to the contact tip and other feeding problems.

SThe most common shielding gas for MIG welding aluminum is 100% argon. Flow rates of 20 to 30 CFH [cubic feet per hour (0.57 to 0.85 m3/hr)] are acceptable. C25 or argon CO2 shielding gases are not acceptable.

OM-226 857 Page 19

Image 23
Contents Description File Wire FeederOM-226 857B ProcessesProtect Your Investment From Hobart to YouTable of Contents Page HOT Parts can burn Symbol UsageArc Welding Hazards Electric Shock can killFlying Metal or Dirt can injure eyes Fumes and Gases can be hazardousARC Rays can burn eyes and skin Welding can cause fire or explosionMoving Parts can injure Welding Wire can injureFire or Explosion hazard Falling Equipment can injureAbout Implanted Medical Devices Principal Safety StandardsCalifornia Proposition 65 Warnings EMF InformationUNE Décharge Électrique peut entraîner la mort Symboles utilisésLE Soudage peut provoquer un incendie ou une explosion LES Pièces Chaudes peuvent provoquer des brûluresLES Fumées ET LES GAZ peuvent être dangereux LA Chute DE L’ÉQUIPEMENT peut provoquer des blessures LE Bruit peut endommager l’ouïeLES Bouteilles peuvent exploser si elles sont endommagées Risque D’INCENDIE OULE Soudage À L’ARC risque de provoquer des interférences Proposition californienne 65 AvertissementsLes Pièces Mobiles peuvent causer des blessures LES Fils DE Soudage peuvent provoquer des blessuresEn ce qui concerne les implants médicaux Principales normes de sécuritéInformations relatives aux CEM OM-226 857 Approximate Cooling Maximum Spool Weld Circuit Overall Specifications For Spool GunComponents Supplied With Spool Gun Conversion Kit Operation Turn off and disconnect in- put powerTurn off and disconnect input power Connecting Spool Gun To Welding Power SourceScrew rotation clockwise decreases Installing Wire Spool And Threading Welding WireRemoving Existing Barrel And Installing Contact Adapter Controls Routine MaintenanceChanging Lower Drive Roll Changing Drive RollsChanging Push Roll Changing Liner TroubleshootingWelding Techniques Gmaw MIG Aluminum Welding HintsBefore You Start Welding Contact Tube Position And Tip-To-Work Distance Common Problems/Troubleshooting− Electrical Diagrams − Parts List Optional Hardware is common and not available unless listed Push Roll .047 1.2 mm Page Assistance ServiceSupport Hobart Welding Products Contact your Distributor for