Hobart Welding Products 210 manual Typical MIG Process Control Settings, Thickness to Amperage a

Page 35

9-2. Typical MIG Process Control Settings

NOTE

These settings are guidelines only. Material and wire type, joint design, fitup, position, shielding gas, etc. affect settings. Test welds to be sure they comply to specifications.

Material thickness determines weld parameters.

1/8 or 0.125 inConvert Material

Thickness to

Amperage (A)

(0.001 in = 1 ampere)

0.125 in = 125 A

.035 in

Wire Size

Amperage Range

 

 

 

 

0.023 in

 

30 − 90 A

0.030 in

40 − 145 A

0.035 in

50 − 180 A

 

 

 

 

 

 

 

 

 

 

 

 

Select Wire Size

 

 

Wire

Recommendation

 

Wire Speed

Select Wire Speed

 

 

Size

 

(Approx.)

(Amperage)

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

0.023 in

3.5 in per ampere

3.5 x 125 A = 437 ipm

125 A based on 1/8 in

 

 

0.030 in

2 in per ampere

2 x 125 A = 250 ipm

material thickness

 

 

0.035 in

1.6 in per ampere

1.6 x 125 A = 200 ipm

 

 

 

 

 

 

 

 

 

 

 

ipm = inches per minute

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

Low voltage: wire stubs into work

Select Voltage

 

 

 

High voltage: arc is unstable (spatter)

 

 

 

 

 

 

 

Set voltage midway between high/low voltage

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

Wire speed (amperage) controls weld penetration (wire speed = burn-off rate)

Voltage controls height and width of weld bead.

Ref. 804 685-A

OM-227 978 Page 31

Image 35
Contents 2006−12 OM-227 978AProcesses DescriptionFrom Hobart to You Table of Contents − Parts List Electric Shock can kill Symbol UsageMarks a special safety message Arc Welding HazardsBuildup of GAS can injure or kill ARC Rays can burn eyes and skinWelding can cause fire or explosion Flying Metal can injure eyesCalifornia Proposition 65 Warnings About Pacemakers Principal Safety StandardsEMF Information Indique un message de sécurité particulier UNE Décharge Électrique peut entraîner la mortLES Fumées ET LES GAZ peuvent être dangereux DES Pièces Chaudes peuvent provoquer des brûlures graves LE Soudage peut provoquer unIncendie ou une explosion DES Particules Volantes peuvent blesser les yeuxDES Organes Mobiles peuvent provoquer des blessures Risque D’INCENDIE OU D’EXPLOLA Chute DE L’APPAREIL peut blesser ’EMPLOI Excessif peut SUREn ce qui concerne les stimulateurs cardiaques Principales normes de sécurité− Definitions − SpecificationsSymbols And Definitions SpecificationsOutput Duty Cycle And OverheatingVolt-Ampere Curves AmperesInstalling Work Clamp − InstallationInstalling Welding Gun Changing Polarity Process/Polarity TableInstalling Gas Supply First, and never to a line ter- minal Selecting a Location And Connecting Input PowerDo not move or operate unit where it could tip Installing Wire Spool And Adjusting Hub Tension Electrical Service GuideFlux Nozzle Installing Contact Tip And NozzleAppropriate setting Connecting Optional Spool GunHold wire tightly to keep it from unraveling Threading Welding WireControls − OperationWeld Parameter Chart For 230 VAC Model 227 949-A Drive Motor Protection − Maintenance &TROUBLESHOOTINGRoutine Maintenance Overload ProtectionReplacing Gun Contact Tip Changing Drive Roll Or Wire Inlet GuideTurn Off power before replacing contact tip To Reassemble Gun Cleaning Or Replacing Gun LinerDisconnect gun from unit Replacing Switch And/Or Head Tube Does not run Troubleshooting TableTrouble Remedy OM-227 978 Circuit Diagram − Electrical Diagram227 951-A Typical MIG Process Connections − MIG Welding Gmaw GuidelinesAmperage Typical MIG Process Control SettingsWire Size Amperage Range Thickness to Amperage aHolding And Positioning Welding Gun Conditions That Affect Weld Bead Shape Cored wireGun Movement During Welding Poor Weld Bead CharacteristicsGood Weld Bead Characteristics Possible Causes Corrective Actions Troubleshooting − Excessive SpatterTroubleshooting − Porosity Troubleshooting − Excessive PenetrationTroubleshooting − Burn-Through Troubleshooting − Lack Of PenetrationTroubleshooting − Incomplete Fusion Application Troubleshooting − Waviness Of BeadTroubleshooting − Distortion Common MIG Shielding GasesWire does not feed Troubleshooting Guide For Semiautomatic Welding EquipmentOM-227 978 Main Assembly − Parts ListDia Part Description Quantity Dia Part Description Quantity Mkgs 231 H-14 GunConsumables Optional Drive RollsOptions Page Work like a Pro Assistance ServiceSupport Hobart Welding Products Contact your Distributor for