Lincoln Electric C2.410 manual Fillet Welds, Lap Welds

Page 21

Fillet Welds

FlatHorizontal Vertical (welded down)

Also see High Deposition Procedures on page 28 for 14 to 10 gauge fillet welds with Jetweld electrodes.

Plate Size

18ga

16ga

14ga

12ga

10ga

 

 

 

 

 

 

Electrode/AWS Class

 

Fleetweld 37/ E6013

 

Diameter (in.)

3/32

1/8

5/32

5/32

3/16

 

 

 

 

 

 

Position(1)

 

0-30° Downhill(5)

 

Current (Amps)

70

105

155

160

210

Polarity(2)

AC

AC

AC

AC

AC

Arc Speed - In./Min.(3) (4)

15

16

17

16

16

Lbs of Elec./Ft. of Weld

.045

.053

.071

.079

.110

 

 

 

 

 

 

Position(1)

 

30-90° Downhill

 

Current (Amps)

75

115

165

170

225

Polarity(2)

AC

AC

AC

AC

AC

Arc Speed In./Min.(3) (4)

16

19

21

20

18

Lbs. of Elec./Ft. of Weld

.042

.049

.062

.070

.100

 

 

 

 

 

 

Lap Welds

Flat

 

 

 

 

 

 

Vertical (welded down)

Plate Size

 

18ga

 

16ga

 

14ga

 

12ga

 

10ga

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

Electrode/AWS Class

 

 

 

 

Fleetweld 37/ E6013

 

Diameter (in.)

 

 

 

 

 

 

 

 

 

 

 

 

3/32

 

1/8

 

1/8

 

5/32

 

5/32

 

 

 

 

 

 

 

 

 

 

 

Position(1)

 

 

 

 

0-30° Downhill

 

Current (Amps)

 

75

115

 

120

165

 

170

Polarity(2)

 

 

AC

 

AC

 

AC

 

AC

AC

Arc Speed - In./Min.(3) (4)

 

17

18

 

16

16

 

12

Lbs of Elec./Ft. of Weld

 

.042

.055

 

.075

.085

 

.110

 

 

 

 

 

 

 

 

 

 

 

Position(1)

 

 

 

 

30-90° Downhill

 

Current (Amps)

 

85

125

 

130

 

185

 

180

Polarity(2)

 

 

AC

 

AC

 

AC

 

AC

AC

Arc Speed In./Min.(3) (4)

 

21

22

 

21

 

21

 

14

Lbs. of Elec./Ft. of Weld

 

.038

.050

 

.061

 

.069

 

.100

 

 

 

 

 

 

 

 

 

 

 

 

(4)Faster arc speeds can be obtained with Fleetweld 7 using DC- polarity and these currents.

-21-

Image 21
Contents Stick Electrode Welding Guide Page Table of Contents Out-Of-Position Welding Vertical and Overhead Welding ProceduresVertical Up Techniques for Fillet and Groove Welds Vertical Down Welds Vertical Up Groove WeldsVertical Up Fillet Welds 160 PolarityWeld Jetweld LH-3800 E7028H8 High-Deposition WeldingWrong End view Side view Corner Welds Groove Welds Groove Welds First PassJetweld 2 E6027 Amps. AC at 14/Min Over E6011 Root Passes Deep Groove Welds Joint a Pass E6011TPlate Size T 14 ga 12 ga 10 ga No. of Passes Leg Size L Flat Fillet WeldsFt. of Weld/Hr Lbs. of Elec./Ft. 049 082 117 162 WeldHorizontal Fillet Welds Welding Inclined Plate Downhill Angle deg Polarity Arc Speed In./Min.3 Lbs. of Elec./Ft.180 Alternate High Speed Welding Sheet MetalPage Edge Welds Lap Welds Fillet WeldsCurrent Amps 110 155 Polarity Diameter PositionCurrent Amps 120 170 Polarity 018 028Roof Deck Thickness 22 ga 20 ga 18 ga 16 ga Burnthrough Spot Welds Roof Decking to Beam Roof Beam FlangeE7018-1 Low Hydrogen WeldingMultipass Page Diameter Current Amps 155 Polarity Overhead Groove WeldsNo. of Pass Leg Size L Overhead Fillet Welds Also see Out-of Position Procedures,Arc Speed In./Min Ft. of Weld/Hr Lbs. of Elec./Ft. No. of Passes Leg Size LBack gouge first bead as needed Plate Size T No. of Passes Horizontal Groove WeldsDiameter Current Amps 230 200 Polarity Arc Speed In./Min Ft. of Weld/Hr Lbs. of Elec./Ft. of Weld230 200 Polarity Use steel backing as onWith E7028 Electrode With E7018 Electrode 275 350132 195 272 409 727 157 236 320 260 335Ft. of Weld/Hr.2 Lbs. of Elec./Ft. 203 335785 Minimum Preheat and Interpass Temperature1 Out-of-Position Group Stick Electrode Typical Operating ProceduresHigh Speed Group High Deposition GroupLow Hydrogen, Low Alloy Steel Group Low Hydrogen GroupFleetweld 5P Shield-Arc Fleetweld 5P+ Fleetweld JetweldFleetweld Fleetweld 35LS Jetweld Shield-Arc 70+ Shield-Arc HYP+Electric Shock can kill Fumes and Gases can be dangerous For Electrically powered Electric and Magnetic Fields Stick C2.410 12/04