Lincoln Electric IM10074 manual Overhead Welding, Hardfacing To Reduce Wear, Welding Sheet Metal

Page 28

b-14

OPERATION

b-14

 

 

 

Overhead Welding

Various techniques are used for overhead welding. However, in the interest of simplicity for the inexperi- enced welder, the following technique will probably take care of his needs for overhead welding:

1.Use 1/8” (3.2mm) 90-105 A or 3/32” (2.5mm) 70 A AWS 6011 electrode on AC.

2.Put the electrode in he holder so it sticks straight out.

3.Hold the electrode at an angle approximately 30° off vertical, both seen from the side and seen from end. (See drawing below.)

Side View

End View

4.Move rapidly enough to stay ahead of the molten slag. A whipping technique may be used to further minimize burn through.

5.If you have a choice, use lap joints rather than fil- lets or butts; the double thickness effect of a lap joint makes it much easier to weld without burning through.

Hardfacing (To Reduce Wear)

There are several kinds of wear. The two most often encountered are:

1.Metal to Ground Wear: Plowshares, bulldozer blades, buckets, cultivator shares, and other metal parts moving in the soil.

2.Metal to Metal Wear: Trunnions, shafts, rollers and idlers, crane and mine car wheels, etc.

30°

30°

It is important to hold a VERY SHORT arc. (A long arc will result in falling molten metal; a short arc will make the metal stay.)

If necessary, and this is dictated by the appearance of the molten puddle, a slight back and forth whipping technique may be used to prevent “dripping”.

Welding Sheet Metal

Welding sheet metal presents an additional problem- burn through. Follow these simple rules:

1.Hold a very short arc. This, together with the prop- er travel speed, will eliminate burn through.

2.Use 1/8” (3.2mm) or 3/32” (2.5mm) AWS 6011.

3.Use low amperage. 75 A for 1/8” (3.2mm) elec- trode, 70 A for 3/32” (2.5mm) electrode.

Each of these types of wear demands a different kind of hardfacing electrode.

When applying the proper electrode, the service life of the part will in most cases be more than double. For instance, hardfacing of plowshares results in 3-5 times more acreage plowed.

How to Hardface the Sharp Edge (Metal to Ground Wear)

1.Grind the share, approximately one inch along the edge, so the metal is bright and clean.

2.Place the share on an incline of approximately 20-30°. The easiest way to do this is to put one end of the share on a brick. (See drawings) Most users will want to hardface the underside of the share, but some might find that the wear is on the top side. The important thing is to hardface the side that wears.

3.Use 1/8” (3.2mm) Wearshield at 80-100 A. Strike the arc about one inch from the sharp edge.

bULLDOG™ 5500

Image 28
Contents Safety Depends on You BulldogSafety California Proposition 65 WarningsElectric Shock can kill Welding and Cutting Sparks can Cause fire or explosion IiiPrécautions DE Sûreté Sûreté Pour Soudage a L’ArcPlease Examine Carton and Equipment For Damage Immediately On-Line Product RegistrationTable of Contents Installation Safety Precautions Location and VentilationStoring Engine Exhaust can killPRE-OPERATION Engine Service StackingTilting OILElectrical Output Connections Welding CAbLE ConnectionsTAbLE A.1 Recommended Welding CAbLE SIzE and Length Hour Meter5INSTALLATIONA-5 Auxiliary Power ReceptaclesElectrical Connections Machine GroundingPremises Wiring Circuit bREAKERSElectrical Device USE with this Product TAbLE A.2Type Common Electrical Devices Possible Concerns Operation WELDER/GENERATOR Controls LimitationsOutput Panel Controls Engine Operation Gasoline Engine ControlsBEFORE Starting the Engine Starting the EngineGenerator Operation Stopping the EngineRunning the Engine LOW OIL SensingGenerator Power Applications TAbLE b.1Welding Operation Control Function / Operation Current Control DialTo USE the bULLDOG 5500 for Welding After YOU Finish the WeldMaterial Thickness Electrode Type Size Setting Welding GuidelinesTAbLE b.2 Welding APPLICATIONS/ELECTRODE Selection GuideWhat Happens in the Arc? Welding circuit for Stick shielded metal arc weldingCorrect Welding Position Correct Way to Strike An ArcCorrect Arc Length Correct Welding SpeedCommon Metals PracticeTypes of Welds Fillet Joints PenetrationMultiple Pass Welds Welding in the Vertical PositionVertical-Up Welding Vertical-Down WeldingHow to Hardface the Sharp Edge Metal to Ground Wear Overhead WeldingHardfacing To Reduce Wear Welding Sheet MetalWelding Cast Iron Cast Iron Plate PreparationOut-of-Position Group AWS E6011 High-Speed Group AWS E6013 Selecting ElectrodesLow Hydrogen Group AWS E7018 OPTIONS/ACCESSORIES AccessoriesLincoln Electric Accessories Routine and Periodic Maintenance MaintenanceEngine Maintenance Engine Adjustments Figure D.2 Clean AreaEngine Maintenance Parts Spark Plug ServiceOperational Clearance Part KohlerGENERATOR/WELDER Maintenance Figure D.6. bRUSH Removal and ReplacementFigure D.7. Major Component Locations 1TROUbLESHOOTINGE-1 PRObLEMS POSSIbLE SymptomsTROUbLESHOOTING Engine requires service to head, head gasket, and/or valves Diagrams Dimension Print M22563BULLDOG Precaucion Warnung