8-2. Typical MIG Process Control Settings

NOTE

These settings are guidelines only. Material and wire type, joint design, fitup, position, shielding gas, etc. affect settings. Test welds to be sure they comply to specifications.

Material thickness determines weld parameters.

1/8 or 0.125 inConvert Material

Thickness to

Amperage (A)

(0.001 in = 1 ampere)

0.125 in = 125 A

.035 in

Wire Size

Amperage Range

 

 

 

 

0.023 in

 

30 − 90 A

0.030 in

40 − 145 A

0.035 in

50 − 180 A

 

 

 

 

 

 

 

 

 

 

 

 

Select Wire Size

Wire

Recommendation

Wire Speed

Select Wire Speed

Size

(Approx.)

(Amperage)

 

 

 

 

 

0.023 in

3.5 in per ampere

3.5 x 125 A = 437 ipm

125 A based on 1/8 in

 

 

 

0.030 in

2 in per ampere

2 x 125 A = 250 ipm

material thickness

0.035 in

1.6 in per ampere

1.6 x 125 A = 200 ipm

 

 

 

 

 

ipm = inches per minute

 

Low voltage: wire stubs into work

Select Voltage

 

High voltage: arc is unstable (spatter)

 

 

 

Set voltage midway between high/low voltage

 

 

 

 

 

 

 

Voltage controls height and width of weld bead.

Wire speed (amperage) controls weld pe- netration (wire speed = burn-off rate)

Ref. 802 439-A

OM-944 Page 32

Return To Table Of Contents

Image 36
Contents OM-944 ProcessesDescription From Hobart to You Table of Contents Options and Accessories Warranty Symbol Usage Marks a special safety messageArc Welding Hazards Electric Shock can killARC Rays can burn eyes and skin Welding can cause fire or explosionFlying Metal can injure eyes Buildup of GAS can injure or killCalifornia Proposition 65 Warnings Principal Safety Standards EMF InformationAbout Pacemakers Identifie un message de sécurité particulier − Consignes DE Sécurité − À Lire Avant UtilisationLE Soudage peut causer un incen- die ou une explosion LES Particules Projetées peu- vent blesser les yeuxLES Pièces Chaudes peuvent cau- ser des brûlures graves LE Bruit peut affecter l’ouïeRisque D’INCENDIE OU D’EXPLO LA Chute DE L’APPAREIL peut blesser’EMPLOI Excessif peut Faire LES Pièces Mobiles peuvent cau- ser des blessuresPrincipales normes de sécurité Information sur les champs électromagnétiquesConsignes relatives aux stimulateurs cardiaques − Specifications SpecificationsVAC Model Duty Cycle And Overheating OutputDuty Cycle % Output AmperesVolt-Ampere Curves Load Amps− Installation Installing Welding Gun Installing Work ClampProcess/Polarity Table Changing PolarityInstalling Gas Supply Rating Label Do not move or operate unit where it could tip = GND/PEElectrical Service Guide For 230 VAC Model Installing Wire Spool And Adjusting Hub TensionThreading Welding Wire Hold wire tightly to keep it from unraveling− Operation ControlsWeld Parameter Chart For 115 VAC Model Welding GuideFor 115 Volt Wire Welding Package Weld Parameter Chart For 230 VAC Model For 230 Volt Wire Welding Package − Maintenance &TROUBLESHOOTING Routine MaintenanceDisconnect power before maintaining Overload Protection Drive Motor ProtectionChanging Drive Roll Or Wire Inlet Guide Turn Off power before replacing contact tipReplacing Gun Contact Tip Cleaning Or Replacing Gun Liner Disconnect gun from unitTo Reassemble Gun Replacing Switch And/Or Head Tube Troubleshooting Table Trouble Remedy− Electrical Diagram Circuit Diagram For 115 VAC ModelCircuit Diagram For 230 VAC Model − MIG Welding Gmaw Guidelines Typical MIG Process ConnectionsTypical MIG Process Control Settings Wire Size Amperage RangeThickness to Amperage a Select VoltageHolding And Positioning Welding Gun Conditions That Affect Weld Bead Shape Poor Weld Bead Characteristics Good Weld Bead CharacteristicsGun Movement During Welding Troubleshooting − Excessive Spatter Troubleshooting − PorosityTroubleshooting − Excessive Penetration Possible Causes Corrective ActionsTroubleshooting − Lack Of Penetration Troubleshooting − Incomplete FusionTroubleshooting − Burn-Through Troubleshooting − Waviness Of Bead Troubleshooting − DistortionTroubleshooting Guide For Semiautomatic Welding Equipment Common MIG Shielding GasesApplication Welding arc not stable Wire slipping in drive rolls Return To Table Of Contents − Parts List Main AssemblyDia Part H-10 Gun Optional Drive Rolls Options195 Page Service SupportContact your Distributor for Hobart Welding Products