LEARNING TO WELD

 

B-17

 

 

 

 

4.After you strike the arc, practice the correct electri- cal stickout. Learn to distinguish it by its sound.

5.When you are sure that you can hold the correct electrical stickout, with a smooth “crackling” arc, start moving. Look at the molten puddle constantly.

6.Run beads on a flat plate. Run them parallel to the top edge (the edge farthest away from you). This gives you practice in running straight welds, and also gives you an easy way to check your progress. The 10th weld will look considerably bet- ter than the first weld. By constantly checking on your mistakes and your progress, welding will soon be a matter of routine.

TROUBLESHOOTING WELDS

Good welds have excellent appearance.

To Eliminate Porosity (in order of importance):

1.Turn on gas supply, if used

2.Decrease voltage.

3.Increase stickout.

4.Increase WFS (wire feed speed).

5.Decrease drag angle.

6.Decrease travel speed.

NOTE: Always be sure the joint is free from moisture, oil, rust, paint or other contaminants.

To Eliminate a Ropy Convex Bead (in order of importance):

1. Increase voltage

2.Decrease stickout.

3.Decrease WFS (wire feed speed.

4.Decrease travel speed.

5.Decrease drag angle.

6.Check for correct gas, if used.

To Reduce Spatter (in order of importance):

1.Increase voltage.

2.Increase drag angle.

3.Decrease stickout.

4.Increase WFS (wire feed speed).

5.Decrease travel speed.

6.Check for correct gas, if used.

To Correct Poor Penetration (in order of impor- tance):

1.Decrease stickout.

2.Increase WFS (wire feed speed).

3.Increase voltage.

4.Decrease speed.

5.Decrease drag angle.

6.Check for correct gas, if used.

If Arc Blow Occurs (in order of importance):

NOTE: Try different ground connection locations before adjusting procedures.

1.Decrease drag angle.

2.Increase stickout.

3.Decrease voltage.

4.Decrease WFS (wire feed speed.

5.Decrease travel speed.

To Eliminate Stubbing* (in order of importance):

1.Increase voltage

2.Decrease WFS (wire feed speed)

3.Decrease stickout

4.Increase drag angle

*Stubbing occurs when the electrode drives through the molten puddle and hits the bottom plate tending to push the gun up.

SP-125 PLUS

Page 31
Image 31
Lincoln Electric IM536-D manual Troubleshooting Welds, To Eliminate a Ropy Convex Bead in order of importance