Lincoln Electric LTW1 manual Troubleshooting Welds

Page 12

11

LEARNING TO WELD

11

 

 

 

TROUBLESHOOTING WELDS

Good welds have excellent appearance.

To Eliminate Porosity (In order of priority):

1.Check for proper gas flow and reset WFS & Volts on chart inside door.

2.Clean joints from moisture, paint, rust etc.

3.Decrease CTWD with GMAW.

4.Decrease drag angle.

5.Decrease travel speed.

NOTE: Always be sure the joint is free from moisture, oil, rust, paint or other contaminant’s.

To Eliminate a Ropy Convex Bead (In order of priority):

1.Check or reset WFS & Volts on chart inside door.

2.Decrease CTWD.

3.Decrease travel speed.

4.Decrease drag angle.

To Reduce Spatter (in order of importance):

1.Check or reset WFS & Volts on chart inside door.

2.Increase drag angle.

3.Decrease CTWD.

4.Decrease travel speed.

To Correct Poor Penetration (In order of priority):

1.Check or reset WFS & Volts on chart inside door.

2.Decrease CTWD.

3.Decrease speed.

4.Decrease drag angle.

If Arc Blow Occurs* (In order of priority):

NOTE: Try different work connection locations before adjusting procedures.

1.Check or reset WFS & Volts on chart inside door.

2.Decrease drag angle.

3.Increase CTWD or weld in opposite direction.

4.Decrease travel speed.

*Arc blow is the effect of a magnetic field which forces the arc from its normal path visual results are concave face uneven leg lengths heavy spatter and porosity.

To Eliminate Stubbing** (In order of priority):

1.Check or reset WFS & Volts on chart inside door.

2.Decrease CTWD.

3.Increase drag angle.

**Stubbing occurs when the electrode drives through the molten puddle and hits the bottom plate tending to push the gun up.

Proper Gun Handling

Most feeding problems are caused by improper han- dling of the gun cable or electrodes.

1.Do not kink or pull the gun around sharp corners.

2.Keep the gun cable as straight as practical when welding.

3.Do not allow dolly wheels or trucks to run over the cables.

4.Keep the cable clean.

5.Innershield electrode has proper surface lubrica- tion. Use only clean, rust-free electrode.

6.Replace contact tip when it becomes worn or the end is fused or deformed.

Image 12
Contents Learning to Weld Aprendiendo a Soldar Apprenez À Souder Table of Contents Learning to Weld ARC-WELDING CircuitSELF-SHIELDED Fcaw Flux Core ARC Welding Gmaw GAS Metal ARC WeldingProcess Selection Common MetalsJoint Types and Positions Welding In The Vertical Position PenetrationFillet Joints Machine SET UP for SELF-SHIELDED Fcaw Process Welding Techniques for the SELF- Shielded Fcaw ProcessVertical-down Welding Correct Welding PositionCorrect Contact Tip to Work Distance Ctwd Correct Welding Speed Travel SpeedHelpful Hints PracticeBack-Stepping Machine SET UP for the Gmaw MIG Process Welding Techniques for the Gmaw MIG ProcessContact Tip to Work Distance Ctwd Correct Welding SpeedTroubleshooting Welds Contenido Aprendiendo a Soldar Circuito DE Soldadura POR ArcoAprendiendo a Soldar Soldadura DE Arco Tubular Fcaw Soldadura DE Arco Metálico CON GAS Gmaw¡Importante Selección DEL Proceso Metales ComunesTipos DE Unión Y Posiciones Soldadura en Posición Vertical PenetraciónSoldadura de Filete Soldadura Vertical Descendente Posición Correcta para SoldarVelocidad Correcta de Soldadura Velocidad de Desplazamiento Consejos Útiles PrácticaMétodo de Pasos en Retroceso Configuración DE LA Máquina Para EL Proceso Gmaw MIG Velocidad Correcta de Soldadura FIGURA19Aprendiendo a Soldar Localizacion DE Averías EN Soldaduras Table DES Matières Apprentisage du SoudageApprenez À Souder Apprentissage DU Soudage LE Circuit DE Soudage À LarcGmaw Soudage a L’ARC Metal GAZ Technique DE PousséeApprenez À Souder Sélection DU ProcédéMétaux Communs Types DE Joints ET PositionsSoudage en Position Verticale PénétrationJoints en Filet Réglage DE LA Machine Pour LE Procédé Fcaw Auto Blindé Soudage en Position Verticale DescendanteLa Position de Soudage Correcte La Vitesse de Soudage Correcte Vitesse de Déplacement 8APPRENEZ À SOUDER8 Indications UtilesPratique Techniques DE Soudage Pour LE Procédé Gmaw MIG La bonne façon damorcer larcIndications Utiles La Vitesse de Soudage CorrecteApprenez À Souder Solution DES Problèmes DE Soudure Pour Éliminer la Porosité par ordre de prioritéPour Réduire les Éclaboussures par ordre d’importance