8-14. Troubleshooting − Waviness Of Bead
Waviness Of Bead − weld metal that is not parallel and does not cover joint formed by base metal.
Possible Causes | Corrective Actions |
|
|
Welding wire extends too far out of nozzle. | Be sure welding wire extends not more than 1/2 in (13 mm) beyond nozzle. |
|
|
Unsteady hand. | Support hand on solid surface or use two hands. |
|
|
8-15. Troubleshooting − Distortion
|
|
| Distortion − contraction of weld metal during welding that forces |
|
|
| base metal to move. |
|
| Base metal moves | |
| |||
|
| ||
|
| in the direction of | |
|
| the weld bead. | |
|
|
| |
|
|
|
|
Possible Causes |
|
| Corrective Actions |
|
|
|
|
Excessive heat input. |
|
| Use restraint (clamp) to hold base metal in position. |
|
|
|
|
|
|
| Make tack welds along joint before starting welding operation. |
|
|
|
|
|
|
| Select lower voltage range and/or reduce wire feed speed. |
|
|
|
|
|
|
| Increase travel speed. |
|
|
|
|
|
|
| Weld in small segments and allow cooling between welds. |
|
|
|
|